FTS-TD-104REV A · NOVEMBER 2026
Chemical Compatibility Screening Matrix
Hose tube and metal hose materials · by chemical family
A first screen of hose and metal hose materials by chemical family. Ratings change with concentration, temperature, aeration and contaminants. Always send the chemical name, concentration and temperature; Patriot FTS checks every application against the hose maker’s resistance data before quoting.
G Generally suitableC Conditional: depends on concentration, temperature or aerationN Not recommended– No screening rating; send details
| Chemical family | UHMWPE / XLPE | PTFE | 304L | 321 | 316L | Monel 400 | C276 | 625 | Bronze |
|---|---|---|---|---|---|---|---|---|---|
| Fresh water, condensate | G | G | G | G | G | G | G | G | G |
| Seawater, brackish water, chloride brines | G | G | C | C | C | G | G | G | – |
| Hydrochloric acid | G | G | N | N | N | C | G | C | – |
| Sulfuric acid, dilute | G | G | N | – | C | C | G | C | – |
| Nitric acid | C | G | G | G | G | C | G | G | – |
| Phosphoric acid | G | G | G | G | G | – | G | G | – |
| Hydrofluoric acid | G | G | – | – | – | G | – | – | – |
| Caustic soda, caustic potash | G | G | – | – | – | G | – | – | – |
| Chlorine | – | G | – | – | – | G | G | – | – |
| Ammonia | – | G | – | – | – | C | – | – | N |
| Aromatic and chlorinated solvents | C | G | – | – | – | – | – | – | – |
| Sour gas, H2S | – | – | – | – | – | – | G | G | – |
| Temperature above 400°F | N | N | C | G | C | C | – | G | – |
Basis and notes
| Item | Note |
|---|---|
| Seawater, chlorides | 316L has a critical pitting temperature of 59°F in ferric chloride; C276 302°F, 625 212°F. For 304L and 321, 316L or a nickel alloy is usually the better choice. Monel resists rapidly flowing seawater; stagnant seawater can cause pitting. |
| Hydrochloric acid | Hydrochloric acid attacks all stainless steels. Monel 400 resists it when de-aerated; aeration and oxidizing salts accelerate attack. Above about 5%, C276 outperforms stainless and handles higher concentrations than 625. |
| Sulfuric acid | 304 resists only about 3% at room temperature; 316 about 20% at room temperature or 3% to 120°F. Monel resists many forms under reducing conditions. |
| Nitric acid | All stainless steels resist nitric acid at room temperature; higher concentrations and temperatures need higher alloys. Polyethylene resists only gentle oxidants, so check strong oxidizing acids. |
| Polyethylene | Not attacked by strong acids or bases. Uncrosslinked polyethylene can dissolve in hot aromatic and chlorinated solvents. Keep media below its boiling point and within −40°F to +250°F. |
| PTFE | Non-reactive with nearly all industrial chemicals; attacked only by reactive metals and fluorinating agents. Use a conductive liner for flammable or low-conductivity fluids. Hose limit −40°F to +400°F by construction. |
| Ammonia | Ammonia causes stress corrosion cracking in copper alloys such as bronze; Monel 400 contains 28–34% copper. |
| Chlorine | The Chlorine Institute recommends Monel 400 and C276 for metallic chlorine hoses; convoluted PTFE is also used for chlorine transfer. |
| Sour service | C276 resists sulfide stress cracking in sour oilfield environments; 625 is used for sour gas with H2S above 150°C. Stainless steels in sour service are governed by the owner’s specification. |