FTS-TD-103REV A · NOVEMBER 2026
Metal Hose Alloy Selection Data
316L · 321 · 304L · Monel 400 · C276 · 625 · Bronze
The seven alloys Patriot FTS builds metal hose with, compared by chemistry, typical reason for selection, temperature and published corrosion data. Use with the chemical screening matrix (FTS-TD-104). We review every application before quoting.
Quick selection
| Alloy | UNS | Key chemistry | Typical reason to choose |
|---|---|---|---|
| 316L stainless | S31603 | 2–3% Mo, 0.030% C max | Chlorides, salt air, many chemicals and cleaning fluids |
| 321 stainless | S32100 | Titanium stabilized | Elevated temperature; cycling through 800–1500°F |
| 304 / 304L stainless | S30400 / S30403 | 18 Cr / 8 Ni, no Mo | General service; standard braid alloy |
| Monel 400 | N04400 | Ni-Cu, 63% Ni min, 28–34% Cu | Seawater, HF acid, caustic, chlorine |
| Hastelloy C276 | N10276 | Ni-Mo-Cr, 15–17% Mo | Strong acids, chlorides and halides, chlorine, sour |
| Inconel 625 | N06625 | Ni-Cr-Mo-Nb, 58% Ni min, 8–10% Mo | High temperature, seawater, sour gas |
| Bronze | – | Copper alloy | HVAC, water, copper tube systems |
Temperature notes
| Material | Published temperature data |
|---|---|
| 321 | Oxidation resistance to 1500°F (816°C); resists intergranular corrosion after 800–1500°F exposure |
| 304 / 304L | Carbides can form at 800–1500°F; 304L preferred for welded assemblies |
| Monel 400 | Good mechanical properties from subzero to about 896°F (480°C) |
| Inconel 625 | Oxidation resistance to 1922°F (1050°C) |
| PTFE-lined hose | −40°F to +400°F, by construction |
| UHMWPE / XLPE hose | −40°F to +250°F |
Pitting and crevice data Higher is better
| Alloy | Critical pitting temp. | Critical crevice temp. | Chloride SCC, boiling MgCl2 |
|---|---|---|---|
| 316L | 59°F | 32°F | Cracked in 2 h |
| Inconel 625 | 212°F | 104°F | No cracking in 1,008 h |
| Hastelloy C276 | 302°F | 131°F | No cracking in 1,008 h |
Published data in acidified 6% ferric chloride (72 h) and stressed U-bends in boiling 45% magnesium chloride.
Choosing among stainless steels
- Chlorides or aggressive chemicals: 316L.
- Sustained heat: 321.
- Neither: 304 / 304L.
- For chlorides beyond 316L, step up to a nickel alloy.
Hose, braid and fittings are separate choices
The corrugated core touches the media; the braid and fittings may be a different alloy. Standard stainless pump connectors use a 321 hose with a 304L braid. If your specification requires one alloy throughout, say so on the request.
The corrugated core touches the media; the braid and fittings may be a different alloy. Standard stainless pump connectors use a 321 hose with a 304L braid. If your specification requires one alloy throughout, say so on the request.
Chlorine service
The Chlorine Institute recommends Monel 400 and Hastelloy C-276 for metallic chlorine hoses; C-276 is generally considered the better option. Above about 5% hydrochloric acid, C-276 is a major improvement over stainless steels and handles higher concentrations better than 625.
The Chlorine Institute recommends Monel 400 and Hastelloy C-276 for metallic chlorine hoses; C-276 is generally considered the better option. Above about 5% hydrochloric acid, C-276 is a major improvement over stainless steels and handles higher concentrations better than 625.